Materials: what the shape of a tank tells you
LCO: the cathode in your phone
LCO is NMC's older sibling: the same layered oxide, but all cobalt. And it rules a different market: almost every phone and laptop runs on it.
- Potential vs Li/Li⁺
- –
- Lithium in the material
- –
- Used up to 4.58 V
- –
- Of that above 4.2 V
- –
Coming from the left, the curve falls evenly from about 4.55 V, then settles at about 3.9 V and barely moves for a good third of the capacity, before it drops off at the very end. In the tank, that's a broad, evenly sloping section deep down, one big reservoir above it, and a narrow neck where the tank is almost full.
Where does the big reservoir come from?
From the same thing that makes LFP flat, just on a smaller scale. Between about Li0.75CoO2 and Li0.94CoO2, two versions of the crystal exist side by side, one richer in lithium and one poorer. While the material switches from one to the other, the level stays put. It's the weir again.
Why push it higher?
Frankly: to extract more capacity. Like NMC, it holds about 274 mAh/g in theory. At 4.2 V you can use only half of that. Charged to 4.58 V, this cell gives about 200 mAh/g. Everything above the line at 4.2 V is extra.
That's the game phone makers play, and they play it aggressively: lots of energy, but not many cycles. A phone only has to last a few hundred cycles, and in a phone the price of cobalt matters far less than in a car, so they trade lifetime for voltage. It's the same game of filling levels as in NMC: every bit of extra voltage empties the tank a little further and brings more capacity. And just like NMC, the structure suffers if you empty it too far.
Sources for this part
- Curve: half-cell measurement (Canrd), high-voltage LCO (4.53 V type), charged at 0.1C to 4.58 V, first discharge at 0.1C, digitised (see Data source at the bottom). Not an open-circuit voltage: the overpotential is still in it. Dashed above the cut-off: extrapolated as a solid-solution tail up to 4.6 V, not measured.
- Reimers and Dahn, Electrochemical and in situ X-ray diffraction studies of lithium intercalation in LixCoO2, Journal of the Electrochemical Society 139 (1992) 2091, doi:10.1149/1.2221184.
Questions, or a material where this doesn't fit? Write me or find me on LinkedIn. All materials side by side: Materials tool.
Data source
All curves in this chapter except graphite and silicon are half-cell measurements by Canrd, published with their materials and used here with their kind permission.